EPDM
EPM – EPDM or Ethylene – Propylene Rubber. EPM can only be vulcanised by peroxides or radiation; whereas EPDM can be vulcanised conventionally using sulphur.
-
Excellent inherent high and low temperature ranges. Typically -49 F to +249 F for standard compounds.
-
Special compoundig can increase some grades to function continually at +284F E.P's are inherently resistant to attack by oxygen, U.V., Ozone and extreme weather environments, and will give long service in these contidions.
-
E.P's do not have good adhesion properties and expert advice should be sought from our Technical Department about bounding applications.
-
Resistance to Chemicals; resistant to many chermicals and solvents. Good resistance to many corrosive chemicals. The performance of E.P's in hot water and high pressure steam is better than in dry heat.
| Ref. |
Specific Gravity |
Hardness |
Tens. Stren. |
Elong. |
Tear. Stren |
Compres. Set |
Working Temp. |
| |
g/cm3 |
Shore A |
psi |
% |
ppi |
C |
h |
% |
F |
| E350 |
1,04 |
30 |
1150 |
640 |
|
70 |
22 |
25 |
-40/230 |
| E450 |
1,07 |
40 |
1300 |
500 |
105 |
70 |
22 |
40 |
-40/230 |
| E550 |
1,17 |
50 |
1300 |
450 |
130 |
70 |
22 |
35 |
-40/239 |
| E602 |
1,30 |
60 |
1000 |
500 |
140 |
70 |
22 |
20 |
-40/248 |
| E646 |
1,16 |
65 |
1550 |
250 |
150 |
100 |
22 |
25 |
-40/285 |
| E647 |
1,16 |
65 |
1450 |
300 |
150 |
70 |
22 |
25 |
-40/248 |
| E715 |
1,16 |
70 |
1450 |
250 |
170 |
70 |
22 |
20 |
-40/248 |
| E701 |
1,31 |
70 |
998 |
300 |
110 |
70 |
22 |
30 |
-40/248 |
| E757 |
1,18 |
75 |
1450 |
225 |
170 |
70 |
22 |
20 |
-40/248 |
| E850 |
1,16 |
80 |
1450 |
225 |
170 |
70 |
22 |
40 |
-31/248 |
| Ref. |
Specific Gravity |
Hardness |
Tens. Stren. |
Elong. |
Tear. Stren |
Compres. Set |
Working Temp. |
| |
g/cm3 |
Shore A |
psi |
% |
ppi |
C |
h |
% |
F |
| E645 |
1,18 |
70 |
1550 |
250 |
150 |
70 |
22 |
20 |
-40/248 |
| E935 |
1,18 |
85 |
1450 |
200 |
170 |
70 |
22 |
48 |
-31/248 |
| Ref. |
Specific Gravity |
Hardness |
Tens. Stren. |
Elong. |
Tear. Stren |
Compres. Set |
Working Temp. |
| |
g/cm3 |
Shore A |
psi |
% |
ppi |
C |
h |
% |
F |
| E566 Green |
1,23 |
60 |
1150 |
350 |
100 |
70 |
22 |
40 |
-40/239 |
| E666 Green |
1,32 |
70 |
1300 |
300 |
130 |
70 |
22 |
40 |
-40/239 |
| E469 White |
1,26 |
50 |
1300 |
400 |
95 |
70 |
22 |
30 |
-40/230 |
| E569 White |
1,25 |
60 |
1150 |
350 |
100 |
70 |
22 |
40 |
-40/239 |
| E669 White |
1,32 |
70 |
1300 |
300 |
130 |
70 |
22 |
40 |
-40/239 |
| E849 White |
1,38 |
80 |
700 |
200 |
110 |
70 |
22 |
60 |
-22/230 |